Sections

Site map →

EN

Spot welding: how the nugget forms and how to check it

Resistance spot welding (process 21 in ISO 4063, RSW) joins overlapping sheets with no filler and no shielding gas. Two water-cooled copper electrodes squeeze the sheets, a high current passes for a fraction of a second, and the metal melts where the sheets touch. It freezes as a small round nugget.

Short answer

Heat comes from current squared × resistance × time (Joule heat), and the setting is a balance of current, weld time and electrode force. The target is a nugget of about 5√t in diameter, where t is the sheet thickness in mm: 5 mm for 1 mm sheet. Electrodes are copper–chromium or copper–chromium–zirconium and have to be dressed as the tip spreads. Too little force or too much current throws metal out (expulsion); too little heat leaves a “stuck” weld with no nugget. Check by peel or chisel test. Zinc-coated steel needs 10–20 % more force and more current, aluminium much more current. For sheet work in general see welding thin sheet.

How the weld forms

The sheet stack is part of the electrical circuit. Current is the same everywhere in it, but heat is released where resistance is highest, and that is the interface between the two sheets, not the contact with the water-cooled copper tips. The metal at the interface melts first, the molten zone grows into a nugget, and the cooled electrodes keep the surface solid.

  1. Squeeze. The electrodes close and bring the force up to the set value before any current flows.
  2. Weld. Current flows for the set time (usually counted in mains cycles); the nugget forms.
  3. Hold. Force stays on with the current off while the nugget solidifies under pressure.
  4. Release. The electrodes open and the sheets move to the next spot.

The joint is a lap joint with access from both sides. It carries load in shear (the sheets pull along the plane) much better than in peel (the sheets are pulled apart at the spot), so the design should avoid peel loading.

Force and current over the four phases of the cycle, and a section of the spot with the nugget between the sheets
Current flows only during the weld, and the force stays on until the end of the hold; the nugget forms where the sheets meet.

Download the diagram: SVG · PNG

Advertisement

Parameters and what each one does

Current, time and force are set together. Moving one moves the window for the others.

Spot welding parameters
ParameterWhat it doesToo lowToo high
Welding currentSets the heat (it enters as the square)Small nugget, or a stuck weld with no fusionExpulsion (splash), deep indentation, fast tip wear
Weld timeHow long the heat is applied; a longer time grows the nugget and spreads heat into the sheetSmall nuggetExpulsion, indentation, heat in the sheet, tip wear
Electrode forcePresses the sheets together, sets contact resistance and holds the molten zoneExpulsion, sticking, short electrode life (contact resistance too high)Deep indentation; lower contact resistance, so less heat and a smaller nugget
Tip face diameterSets contact area and current densityOverheated surface, indentationLower current density: smaller nugget (this is what wear does)
Squeeze timeLets force build up before currentExpulsion at the start, marked surfaceCycle slower, no effect on the weld
Hold timeKeeps the pressure while the nugget freezesSurface splash, sticking, internal cracksCycle slower; electrodes cool the spot longer
Electrode coolingTakes heat out of the tipsShort tip life, sticking—

The wanted result is a margin: a setting where the weld is above the minimum size and still well below expulsion, so that tip wear and sheet variation do not push it out. Starting values for a given material and thickness come from the machine maker’s table or the customer’s specification; this page does not give a schedule.

Nugget diameter: the 5√t rule

TWI gives the target weld diameter as typically 5√t, with t the sheet thickness in mm. Its minimum acceptable size is 70 to 80 % of that target, depending on the application standard. The values below follow from that rule; for sheets of unequal thickness the thinner sheet is normally used.

Spot weld diameter from the 5√t rule (t = sheet thickness)
Sheet thickness t, mmTarget 5√t, mm70–80 % of target, mm
0.63.92.7–3.1
0.84.53.1–3.6
1.05.03.5–4.0
1.56.14.3–4.9
2.07.14.9–5.7
3.08.76.1–6.9

The rule is a target, not a code limit. Other sources set the minimum differently: the I-CAR guide for collision repair uses 4.5√t of the thinnest sheet, and automotive and appliance specifications state their own values. Where the drawing or the customer specification gives a minimum size, that figure wins. The weld is measured on a torn-out plug (see testing below), not on the visible dent.

Electrodes: alloy, tip, wear

  • Alloy. Copper–chromium and copper–chromium–zirconium (class 2 in ISO 5182) are the usual choice for low-carbon and high-strength steel. For coated steel the higher-conductivity copper–zirconium or dispersion-strengthened copper heats the surface less and can reduce sticking. Stainless steel is welded with harder class 3 alloys (copper–nickel–silicon) at higher force and lower current. Tungsten–copper and similar refractory tips are for projection welding, not for spot welding.
  • Shape. Truncated-cone tips; for coated steel they last longest. The tip face diameter sets the contact area and so the current density. The electrode body should be at least 2.5–3 times the tip diameter.
  • Wear. The tip mushrooms with every weld, the contact area grows and the same current heats a larger area, so the nugget shrinks. Dress the tip by cutting the cone back to the original diameter, taking off little material; some shops compensate with stepped-up current, set by trial. Keep the tips aligned.
  • Cooling. Poor cooling is the most frequent cause of short electrode life. TWI recommends about 4 l/min through each electrode on thin uncoated sheet and 6 l/min or more on coated and thicker sheet, with water in at no more than 20 °C and out at no more than 30 °C.

Preparation and materials

The surface must conduct current evenly. Heavy oxide, passivated layers, oil or paint raise the contact resistance in a random way; TWI names splash, surface burning and misshapen welds as the result. The usual differences between materials:

Spot welding by material
MaterialWhat changes against bare low-carbon steel
Low-carbon steel, bareThe reference. Class 2 electrodes (CuCr, CuCrZr). Remove oil, thick scale and paint from the contact area.
Zinc-coated steelElectrode force usually 10–20 % higher; 2–3 cycles allowed for the coating to be displaced before the nugget starts; substantially higher current than for bare steel; truncated-cone tips; good cooling; shorter tip life (TWI).
Stainless steelHarder class 3 electrodes (CuNiSi), much higher force and lower current than for carbon steel; stainless has high resistance and low heat conduction.
AluminiumMuch higher current than for steel (high electrical and thermal conductivity, and a resistive oxide film); copper forms an alloy with aluminium, so tip wear is very fast. Needs a strong machine, tip dressing and cleaning of the oxide. Not a job for hand tongs.

The coating on galvanized sheet changes the zinc side of the weld, not the principle: see welding galvanized steel for what zinc does in arc welding, and aluminium for the metal itself.

Defects: causes and fixes

Spot weld defects
DefectCauseWhat to do
Expulsion (splash of molten metal)Current or time too high, force too low, short squeeze time, poor fit-up or a dirty surface, worn or misaligned tipsLower the current or time, raise force, give the sheets a fit with no gap, align and dress the tips
Stuck weld (no nugget, the sheets only “tacked”)Current or time too low, tip too large or worn, shunting from the previous spot, a high-resistance film on the sheetRaise the current, dress the tips, increase the pitch, clean the surface; confirm by peel test
Undersized nuggetTip wear, shunting, low current, mismatch of the tip diameter with the thicknessDress or change the tips, increase the pitch, correct the setting against the table
Electrode sticking to the sheetLow force, short hold, aluminium alloying with the copper (zinc coatings also pick up on the tips), poor coolingCheck cooling, hold time and force; dress the tip; for coated sheet use the electrode alloy made for it
Excessive indentation, burn marksForce, current or time too high; tip too small; surface filmReduce, enlarge the tip face, clean the surface
Interface failure in the peel testSmall weld diameter, lack of fusion, hard brittle nugget, cracking or porosity (TWI)Raise the weld size, check force and splash; for hardenable steels check the weld cycle
Cracks and porosity in the nuggetToo little force or splash, mainly in thick steel (TWI)Higher force, hold time; check with a section

Cracks and porosity inside the nugget are found in thick steel mainly when force is too low or when there is splash. They cannot be seen from outside: only a section or a destructive test shows them.

Checking a spot weld

  • Peel or chisel test. TWI recommends confirming quality by peel or chisel testing. A good weld in ordinary low-carbon steel pulls a plug out of one sheet; the plug diameter is measured and compared with the required size. A weld that separates cleanly at the interface (an interface failure) is rejected: causes include a small weld, lack of fusion, a hard brittle nugget or a joint loaded in shear or torsion.
  • Visual. Even indentation, no cracks or burn marks round the spot, no splash. Excessive indentation points to too much force, current or time.
  • Section. A cut and etched cross-section shows the nugget size and any internal cracks or porosity; it is used for procedure setting and for disputes.
  • First and last spots. In production the setting is checked on a test piece at the start and after tip dressing or a tip change.

The ISO and national standards for spot weld testing are not summarised here: use the one the contract names.

Spot pitch and edge distance

The next spot placed too close to the previous one has a path of lower resistance through the existing nugget. Part of the current is shunted through it and the new nugget comes out smaller. Spacing therefore has a minimum that depends on the thickness, the material and the coating, and it is given in the machine maker’s tables or the design standard. A spot too near the edge of the sheet loses heat and metal and can burst out at the edge. The flange has to be wide enough for the electrode to reach the joint and for the weld to be contained. This page quotes no figures for the minimum pitch or edge distance because none could be confirmed from two independent sources.

Hand spot tongs and industrial machines

Both do the same job, and both are bounded by the same physics; the difference is in how well the three parameters are controlled.

Hand spot welder and industrial machine
Hand spot welder (tongs)Industrial machine
ForceApplied by hand on the lever, not measuredSet and measured: pneumatic or servo gun, bench press-type machine
Current and timeFixed or coarse settings, often set by the triggerSet by a controller; constant-current control and current stepping are common options
CoolingAir, or none; the duty cycle is shortWater through the electrodes and the transformer
MaterialsThin low-carbon sheet; the maker states the limitSteel, coated steel, stainless and aluminium, with tables for each
RepeatabilityDepends on the operatorSame cycle every time; the settings are recorded
Typical useRepair, workshop, hobby, wire and mesh in the home workshopProduction lines, robots, car bodies

The thickness a hand unit can weld is stated by its maker: do not assume that 2 + 2 mm sheet works because 1 + 1 mm does. Welding with a hand unit follows the same rules for surface, cooling of the tips and testing a trial piece.

Where spot welding is used

Process 21 is the standard method for thin sheet assemblies made in large numbers: car bodies and sub-assemblies, appliance housings, cabinets, shelving, ducts and enclosures. It needs no filler, no gas and no weld cleaning, it is quick, and it distorts less than arc welding because the heated volume is small. Its limits are the lap joint with access from both sides, the thickness the machine can weld and the lack of tightness: a spot weld is not a sealed seam (process 22, seam welding, is). In a workshop spot welding competes with MAG plug welds and stitch welds; see thin sheet, MIG/MAG and the process table for the choice.

Standards and references

Where the figures and statements on this page come from. Standards are quoted as cited by TWI; the standard texts themselves were not consulted.

  • ISO 4063, process number 21, resistance spot welding (RSW), in the site’s process table.
  • TWI FAQ: interface failures in resistance spot welds, target diameter 5√t, minimum 70–80 % of target, peel or chisel testing, causes of interface failure.
  • TWI FAQs: electrode material; coated steels; minimising electrode wear; aluminium alloys, electrode classes (ISO 5182 as cited), coated steel force and weld time, body diameter, cooling water flow and temperature, dressing, aluminium current and tip wear; BS 1140 named for guideline conditions.
  • I-CAR Repairability Technical Support Portal, minimum nugget 4.5√t of the thinnest sheet used in collision repair; given to show that minima differ between users.

Frequently asked questions

What does 5√t mean for a spot weld?

It is the usual target diameter of the nugget in millimetres: five times the square root of the sheet thickness in millimetres. For 1 mm sheet that is 5 mm, for 2 mm sheet about 7 mm. The minimum accepted size is lower (TWI: 70–80 % of the target) and the product specification decides it.

Why does the electrode stick to the sheet?

Mostly from too little force or too short a hold time, from poor cooling, or from aluminium (and, on coated sheet, zinc) picking up on the copper tip. Check water flow first, then dress the tip. For zinc-coated sheet an electrode alloy with higher conductivity (copper–zirconium) can reduce sticking.

Can galvanized steel and aluminium be spot welded?

Yes, but with changes. Galvanized steel takes about 10–20 % more force, more current and more frequent tip dressing; aluminium takes much higher current and loses tips quickly. See welding galvanized steel.

How do you test a spot weld in the workshop?

Peel or chisel the sheets apart on a trial piece: a sound weld in ordinary steel tears out a plug, and the plug diameter should reach the required size. A clean break along the interface means the weld is rejected. Do it at the start of a run and after dressing the tips.

What is the difference between spot welding and MIG plug welds?

Spot welding needs access to both sides and no filler, it is fast, and it leaves no weld metal to grind. A MAG plug weld works from one side and fills a hole in the top sheet, so it is the choice where the second side is not reachable. See MIG/MAG and thin sheet.

Can I spot weld with a hand spot welder at home?

On thin low-carbon sheet, yes. The maker states the thickness limit; force and time are not controlled, so test every setup by peeling a trial piece. For aluminium, stainless and anything structural it is the wrong tool.

Author: , welder and metal fabricator Updated: