Which NDT method for which weld: VT, PT, MT, UT or RT

Non-destructive testing (NDT) examines a finished weld without damaging it. Five methods cover almost every case in a workshop and on site: visual (VT), penetrant (PT), magnetic particle (MT), ultrasonic (UT) and radiographic (RT). VT, PT and MT see the surface, UT and RT see the volume.

Short answer

VT comes first and applies to every weld. PT and MT add the surface cracks that the eye misses: MT works only on ferromagnetic steel, PT on any metal with a clean, open surface. UT and RT look inside: UT is the method for planar flaws such as lack of fusion and cracks, RT for pores and inclusions, and it leaves a record. Which method is used and how much of the weld is tested is set by the application standard or the contract, with ISO 17635 as the general rule, not by the welder. Each method has its own acceptance standard, tied to the quality level of ISO 5817 only indirectly. Personnel are certified to ISO 9712 at level 1, 2 or 3.

The five methods in one table

The abbreviations are the same in every language. The standard in the second column describes how the test is carried out; whether an indication is acceptable is decided by a different standard (see below).

NDT methods for welds: what they find and where they stop
MethodStandardFindsMaterialLimits
VT, visualISO 17637Surface: undercut, overlap, spatter, weld shape and sizeAnyNothing inside the metal; depends on light, access and the inspector
PT, penetrantISO 3452-1Cracks and pores that break the surfaceAny metal with a non-porous surface, including austenitic stainless steel and aluminiumOpen defects only; the surface must be clean and dry
MT, magnetic particleISO 17638Surface and near-surface cracksFerromagnetic only: carbon and low-alloy steelNot for austenitic stainless steel or aluminium; the field must cross the flaw
UT, ultrasonicISO 17640Internal: lack of fusion, lack of penetration, cracksMost metals; coarse-grained weld metal is harder to testNeeds access, a written procedure and a skilled operator
RT, radiographicISO 17636-1 (film), ISO 17636-2 (digital)Pores, inclusions, lack of penetration, with a record imageAny; thickness is limited by the sourceRadiation protection, cost, access to both sides; a flaw across the beam can be missed

The first digit of an ISO 6520-1 imperfection number already hints at the method: shape shows to the eye, pores on film, planar flaws under ultrasound. The diagram is on the page ISO 6520 imperfection numbers.

Advertisement

When to use which

  • VT: always, and usually first. It costs nothing but light and a gauge, and a weld with a bad surface is not worth sending for UT or RT. The report is in the visual inspection calculator.
  • A surface crack is suspected. On carbon and low-alloy steel use MT, which also finds flaws just under the surface. On austenitic stainless steel, aluminium or any non-magnetic metal MT does not work, so use PT.
  • A flaw inside the weld is suspected. UT for lack of fusion, lack of penetration and cracks; RT for pores and inclusions, and where a permanent image is required.
  • Several at once. A critical joint is often tested by a surface method and a volume method together, because each misses what the other sees.

The choice for a given weld is made from the quality requirements, material, thickness, welding process and the extent of testing: this is what ISO 17635 guides. Imperfection names and numbers are in the weld defects catalogue.

Acceptance criteria: a separate standard for each method

A test finds an indication; another standard says whether it is allowed. VT is judged directly against the limits of ISO 5817. The other methods have their own acceptance levels:

Where the acceptance limits are
MethodAcceptance standardWhat it sets
VTISO 5817Limits of imperfections for quality levels B, C and D; see the calculator
PTISO 23277Acceptance levels for indications of surface-breaking imperfections
MTISO 23278Acceptance levels for magnetic particle indications
UTISO 11666Acceptance levels for ultrasonic indications
RTISO 10675-1Acceptance levels for radiographic indications in steel

ISO 17635 links the quality level of ISO 5817 to the testing level and the acceptance level of each technique, but the acceptance levels are not a direct translation of the quality levels: they are tied to the overall quality of a batch of welds. Take the pair for your job from the annex of ISO 17635 or from the application standard; this page does not list the pairs.

Who may test: ISO 9712

Testing other than the visual check is done by personnel certified to ISO 9712 for the method, at one of three levels. The certificate is held per method: a level 2 in UT does not cover MT.

  • Level 1 carries out tests following written instructions, under the supervision of level 2 or 3.
  • Level 2 performs and directs testing by established techniques.
  • Level 3 takes responsibility for the test facility and staff and establishes techniques and procedures.

The level required for a given job is named by the application standard or the contract.

How much is tested: set by the standard, not by the method

The extent (which welds, what share of the length) comes from the application standard or the contract and grows with the consequence of failure. Under EN 1090-2 visual examination applies to all welds in every class, and supplementary NDT (MT, PT, UT, RT) follows Table 24, with an extent that grows with the execution class; the first five joints made to a new WPS are tested to twice that extent. The percentages are not quoted here: take them from the edition in force. The classes and what they change are on the page EN 1090 and execution classes; the quality system around them is ISO 3834.

The quality level is fixed by the design documents. A test method does not change that level: it only shows whether the weld meets it.

Standards and references

Where the statements on this page come from. The standard texts were not consulted in full: titles and scopes are as given in the ISO and national catalogues and in the sources named.

  • ISO 17635, general rules for choosing methods, techniques and acceptance levels; the acceptance levels are not a direct translation of the ISO 5817 quality levels (ISO and BSI catalogue descriptions).
  • ISO 17637, 3452-1, 17638, 17640, 17636-1 and -2, technique standards of VT, PT, MT, UT and RT (designations as in the ISO catalogue).
  • ISO 23277, 23278, 11666, 10675-1, acceptance levels of PT, MT, UT and RT (designations as in the ISO catalogue).
  • ISO 9712, certification of NDT personnel, levels 1 to 3, per method (summary in the CSWIP scheme documents).
  • EN 1090-2, Table 24 and clause 12.4.2.2, extent grows with the execution class; the first five joints of a new WPS at twice the extent (TWI Job Knowledge 131); percentages not quoted. See EN 1090.
  • The site’s own NDT table, what each method finds and misses (VT, PT, MT, UT, RT).

Frequently asked questions

Which NDT method finds defects inside a weld?

Ultrasonic (UT) and radiographic (RT) testing. UT is the method for planar flaws such as lack of fusion and cracks, RT shows pores and inclusions and leaves an image as a record. Visual, penetrant and magnetic particle testing see only the surface.

Can magnetic particle testing be used on stainless steel?

Only on grades that are ferromagnetic. Austenitic stainless steel, the common kind, is not, and neither is aluminium: for them use penetrant testing (PT).

Is visual testing enough?

It is the first step and the one test that applies to every weld, but it sees only the surface. Whether it is enough is set by the application standard or the contract. A weld that must be sound inside needs UT or RT as well. See the visual inspection report.

Does NDT change the ISO 5817 quality level?

No. The level comes from the design documents. The test only shows whether the weld meets it, and acceptance of PT, MT, UT and RT indications follows each method’s own standard, linked to the level through ISO 17635 and the application standard.

What do levels 1, 2 and 3 of ISO 9712 mean?

Level 1 tests by written instruction under supervision; level 2 performs and directs testing by established techniques; level 3 is responsible for the facility, the staff and the procedures. The certificate is per method.

How much of the welds has to be tested under EN 1090?

Visual examination covers all welds. Supplementary NDT follows Table 24 of EN 1090-2 and grows with the execution class; the first five joints of a new WPS are tested to twice the extent. Take the percentages from the edition you work to. See EN 1090.

Author: , welder and metal fabricator Updated: