Tungsten blue, black or melting in TIG: what to check, in order
A tungsten that goes blue, black or blobs at the tip is telling you where the shield or the current is wrong. The cause is almost always one of seven things, and most are free to check, so they come first.
Short answer
Check in this order: the gas on the cylinder, the flow and post-flow, the stick-out, the polarity, the current against the diameter, the tungsten type against the current type, then the grind and your hand. Argon at 6–10 l/min, post-flow about 1 s per 10 A, stick-out no longer than the cup diameter, DC− for steel and stainless. A tungsten that touched the pool or the rod is not cleaned by burning: stop and regrind it.
Order of checks: cheapest first
Change one thing at a time. The first three take seconds and cost nothing.
- Read the cylinder label. TIG takes argon (Ar 99.99 in the site gas table). A MAG mix with CO₂ or oxygen eats tungsten.
- Flow and post-flow. Flow at the torch against the range; post-flow about 1 s per 10 A.
- Stick-out and cup.
- Polarity. Torch lead in the DC− socket.
- Current against the diameter, table below.
- Tungsten type against the current (DC or AC).
- Grind and then technique: arc length, rod, touching.
Sign, cause, check, remedy
Find the sign on the tungsten or in the weld, then read across.
| Sign | Cause | How to check | What to do |
|---|---|---|---|
| Tungsten inclusions in the weld, the tip grey or covered with metal, the arc wanders | The tungsten touched the pool or the filler rod | Look at the tip under a light. Metal stuck to it, a ball of different colour, a flattened end. | Stop, regrind (see the section below). Arc length about one electrode diameter; dip the rod into the leading edge of the pool and never into the tungsten. Check the start: lift-arc touches the work, HF does not. |
| Tungsten turns blue and then black, dull, oxidised | Too little gas, a post-flow that is too short, too much stick-out, a draught or a leak | Flow at the torch against 6–10 l/min; post-flow is about 1 s per 10 A (15 s at 150 A). Look for a cracked cup, a loose fitting, a fan in the room. | Raise the flow within the range, lengthen the post-flow, bring the tungsten back so that it sticks out no longer than the cup diameter, screen the work. Do not turn the flow up in a draught; shield the work. |
| The tip melts and drips, a bright ball forms and may fall into the pool | Current too high for the diameter, or reverse polarity (DC+) | Compare the current with the diameter row of the table above. Check the socket the torch lead is in: electrode negative is the working polarity. | Go to the next diameter or reduce the current. Move the lead to the DC− socket. DC+ is practically never used because the tungsten overheats and melts. |
| A black or burnt tip right at the start, or after a few seconds of welding | Not argon in the cylinder (a MAG mix with CO₂ or oxygen), or air in the hose | Read the cylinder label and the regulator; the TIG gas is argon (Ar 99.99). Purge the hose before the first arc; the pre-flow is 0.5–2 s. | Change to argon. Set a pre-flow. For gas selection by process see the shielding gas calculator. |
| The tip cracks, spits or splits on AC | A thoriated tungsten (WT-20, red) on alternating current, or a tip ground to a point on AC | Look at the colour band on the electrode and the current type you selected. The balled shape on AC is a rounded point, not a needle. | Use WP (green), WZ-8 (white) or WL-20 (blue) on AC (colour table). Let the ball form from a lightly rounded tip. |
| The arc wanders, the start is hard, the arc jumps from the side of the tip | The tungsten was ground across the axis, the wrong angle, a worn point or dirt on the grind | Look at the grind marks: they should run along the axis. Check the angle against the current: 15–30° narrow and deep, 60–90° wide. | Regrind lengthwise on a clean wheel kept for tungsten, at the angle for the current. A new tip for every important job. |
| Gas coverage poor even with a good flow: the weld discolours, the tungsten oxidises behind the cup | Stick-out too long for the cup, a cup too small for the current, a blocked or dirty cup | Measure the stick-out against the diameter of the cup. Look into the cup for spatter or a cracked insert. | Shorten the stick-out, fit a larger cup (or a gas lens, which gives a calmer flow), clean the cup. The cup size for the current is in the tungsten calculator. |
The colours and oxide content of each type are in the tungsten colour-code table; the TIG basics are on the TIG welding page.
Current against the diameter
An electrode carries less on AC than on DC−, and a diameter that is too thin for the current melts back into a ball that can fall into the pool. These ranges are the site’s own table; the rod in the last column is the filler diameter that goes with it.
| Diameter, mm | DC−, A | AC, A | Filler rod, mm |
|---|---|---|---|
| 1.0 | 15–80 | 20–60 | 1.0–1.6 |
| 1.6 | 70–150 | 60–120 | 1.6–2.0 |
| 2.0 | 100–200 | 80–160 | 1.6–2.4 |
| 2.4 | 150–250 | 100–180 | 2.0–3.0 |
| 3.2 | 250–400 | 160–250 | 2.4–4.0 |
| 4.0 | 400–500 | 200–320 | 3.0–4.0 |
For example, a 2.4 mm tungsten holds 150–250 A on DC− but 100–180 A on AC. If the tip balls up on a current well inside the range, the cause is probably polarity or gas, not the current. The tungsten calculator works out the diameter, grind angle and cup for your current.
What current and tungsten go with the material
Starting settings by thickness, from the TIG settings table: the tungsten, the DC− current, the filler and the argon flow.
| Thickness, mm | Tungsten, mm | Current DC−, A | Filler, mm | Argon, l/min |
|---|---|---|---|---|
| 0.5–1.0 | 1.0–1.6 | 20–50 | 1.0–1.6 | 5–7 |
| 1.5–2.0 | 1.6 | 50–90 | 1.6 | 6–8 |
| 3.0 | 2.0–2.4 | 90–130 | 2.0–2.4 | 7–9 |
| 4.0–5.0 | 2.4 | 130–180 | 2.4–3.0 | 8–10 |
| 6.0–8.0 | 3.2 | 180–250 | 3.0–4.0 | 10–12 |
The full chart is on TIG settings by thickness; argon flow also in the gas calculator.
After contamination: regrind, do not burn it clean
- Stop and let it cool in the gas. A tungsten in air while hot oxidises at once.
- Cut or break off the contaminated end (the part that is grey, black, blue or has metal stuck to it) with a clean tool.
- Grind lengthwise on a wheel kept for tungsten only. Marks across the axis make the arc wander. A wheel used for steel puts steel dust back on the tip.
- Choose the angle for the current: 15–30° at low current, 30–60° as the compromise, 60–90° for the longest life.
- Restart on a scrap piece, then on the joint. A contaminated bead is ground out before welding on.
AC and aluminium: a separate case
On AC the tip balls up by itself, and that is normal; a small ball on a WP or WZ-8 electrode is the working shape. An oversize ball means too much current for the diameter or too much time on the electrode-positive half-cycle. WT-20 (red, thoriated) cracks and spits on AC; use WP, WZ-8 or WL-20. The aluminium side is on welding aluminium.
Where the figures come from
This page adds no figures of its own. Everything numeric is taken from the tables of this site.
- Current by tungsten diameter and the TIG settings by thickness, the tables on the tungsten colour-code page and on TIG settings by thickness.
- Argon flow, post-flow, pre-flow, stick-out, the TIG welding page and the gas table of the gas calculator.
- ISO 6848, tip colours and oxide contents of the tungsten types, as on the colour-code page.
Frequently asked questions
Why does my tungsten turn blue or black?
It oxidised: too little gas, a post-flow that is too short, a stick-out longer than the cup diameter, or a draught. Check the flow against 6–10 l/min and set the post-flow to about 1 s per 10 A. Regrind the tip before the next weld.
I touched the tungsten to the pool. Can I keep welding?
No. Contamination does not burn off, and it puts tungsten inclusions in the weld. Stop, cut or break off the end and regrind it lengthwise, then try on a scrap piece.
Why does the tungsten melt into a ball on DC?
Either the current is too high for the diameter (see the table above) or the polarity is reversed. On DC+ the tungsten overheats and melts, so TIG on DC runs with the electrode negative.
Which tungsten for AC and which for DC?
AC (aluminium, magnesium): WP (green) or WZ-8 (white), balled tip, or WL-20 (blue). DC− (steel, stainless, copper): WL-20, WC-20 or WT-20. Thoriated WT-20 cracks and spits on AC. See the colour-code table.
What grind angle for which current?
15–30° for low current (easy start, narrow arc, wears quickly), 30–60° as the compromise, 60–90° for the longest life and a wide arc. Grind lengthwise on a wheel kept for tungsten.
Can I use MAG gas for TIG?
No. TIG needs argon (Ar 99.99); CO₂ or oxygen in the gas destroys the tungsten in seconds and the weld oxidises. Check the cylinder label: shielding gas calculator.
Updated: