How to tack: how many, how long and in what order

A tack weld is a short weld that holds the parts in position until the final weld is made. It is not a spot of glue: if it stays in the joint, it becomes part of the weld and has to be sound.

Short answer

Use as few tacks as hold the gap, make them short, flat and well fused, and put them in an order that works against shrinkage: from the middle outwards or from side to side, not from one end to the other. The figure the site gives for thin sheet is a tack every 30–50 mm, the middle first, then both ends, then the middle of each remaining gap. For other work the length and spacing come from the job: the WPS, the drawing or the application standard (EN 1090-2 limits the tack length; take the figure from the edition in force). Grind the ends of a tack that stays in the joint to a taper so the root run melts it, and remove any tack that has cracked.

What tacks are for

  • They fix the gap and the alignment. Squareness, diagonals and the root gap are checked before the first run, when correcting still means breaking one tack and not grinding a weld.
  • They resist shrinkage across the joint. Too few tacks and the joint closes up as the weld cools; too many and the joint is restrained and cracks. Number, length and spacing are set by the sequence (distortion).
  • They carry the part while it is moved, turned or preheated.

A tack is welded as carefully as the weld itself: same cleanliness, same filler, the preheat the WPS requires. Dirt, oil or a coating that is not ground off gives porosity in the tack, and it stays in the joint.

Advertisement

Length and spacing

There is no single rule that holds for every joint. The rules of thumb found in handbooks and forums contradict each other, and the one standard that fixes the length for structural steelwork, EN 1090-2 clause 7.5.7 (as read by TWI Job Knowledge 131), expresses it in relation to the thickness: take the figure from the edition you work to. The table gives what the site already says for each kind of work.

Tacks by kind of work: what the site says
WorkTacksWhere
Thin sheetA tack every 30–50 mm; the middle first, then both ends, then the middle of each remaining gap. Then stitches of 15–25 mmWelding thin sheet
Square tube frameTwo opposite corners first, check the square across both diagonals, then the other twoWelding square tube
Pipe butt jointOn the sides, none at 6 and 12 o’clock; ends ground to a taper; gap checked all round before tackingPipe welding positions
Vertical-up, covered electrodeBoth ends and the middle of a longer seam; the bottom tack ground to a taperWelding vertical up
Structural steel to EN 1090-2Clause 7.5.7 limits the length and covers the tack welding; the figure is not quoted hereEN 1090 and execution classes

In general the thicker and stiffer the joint, the longer and further apart the tacks may be; thin and heat-sensitive material wants short tacks, close together. A tack that is too long is a weld that nobody planned: it cools fast, cracks, or leaves a hump that the root run cannot melt.

Order of tacking

  1. Fit first. Clamp or wedge the parts, check the gap, squareness and diagonals before the first tack.
  2. From the middle outwards. First tack in the middle, then both ends, then the middle of each remaining gap. Tacking in sequence from one end pushes all the shrinkage to the far end.
  3. Across, not along. On frames tack two opposite corners, check the square, then the other two. On a pipe, tack on opposite sides.
  4. Long seams. Tack one end and backstep, or tack the centre and backstep; backstep means short lengths laid against the general direction of travel. The diagram of backstep welding is in welding thin sheet, the reasons in distortion.
  5. Check again after tacking. Gap, alignment, level. A wrong part is cheap to correct while it hangs on tacks.

Tacks in the root and remelting

A tack that stays in a groove joint sits in the root and is meant to be melted by the root run. For that:

  • Make it with the same filler and the preheat of the WPS; a small tack on thick or hardenable steel cools quickly and can crack.
  • Grind both ends to a taper. A run that starts on the hump of a tack starts with cold lap instead of fusion, and a hump in the root is not melted through.
  • Check it by eye before welding over it. A cracked tack is removed completely: later passes do not remove a crack, they can carry it on.
  • A tack too large for the root run to melt through is ground down to size, not welded over.

Who puts in the tacks

A tack that stays in the weld is a weld. On work to a standard such as EN 1090-2 the tack is covered by clause 7.5.7, and TWI notes that the qualification of tacks left in the weld is read differently from company to company. None of the sources consulted for this page says that a tack welder needs a separate ISO 9606-1 test, and none says that one does not. Whether tacking is done by a qualified welder or by a fitter is settled by the application standard, the WPS and the contract or the inspection body. The practical reading is the safe one: let a welder qualified for the joint put in tacks that will stay in it. The qualification itself: welder qualification.

Tack defects

Tack defects, causes and what to do
DefectCauseWhat to do
Crack in the tackFast cooling of a small tack; thick or hardenable steel; a stiff joint; no preheatPreheat as the WPS says; grind the cracked tack out completely and tack again
Lack of fusion at the ends, cold lapHump of the tack, low heat at the start, dirty edgeGrind the ends to a taper, clean, set the current for the tack as for the weld
Porosity in the tackOil, rust, moisture or coating left on the joint; poor gas shieldingClean to bright metal; for zinc-coated steel see welding galvanized steel
Tack breaks when fitting, lifting or heatingToo short, too few, or the clamps pull against the tacksAdd tacks in the sequence, release the clamps before welding, do not use force to close a gap
Gap closes or opens, part movesToo few tacks, wrong order, tacking from one endWedge the gap, tack from the middle, see distortion
Root not melted over the tackTack too large or too high, root gap too narrowGrind to a taper and to a lower height before the root run

The crack in a tack and the lack of root penetration over it are the two that find their way into the finished joint; see lack of penetration and, for how such flaws are found, non-destructive testing.

Standards and references

Where the statements on this page come from. No tack length or spacing formula is given: the handbook rules disagree and the one standard figure was not available in its own text.

  • EN 1090-2, clause 7.5.7, tack welds are covered; the length is limited; qualification of tacks left in the weld is read differently by different companies (TWI Job Knowledge 131, “Fabrication requirements of BS EN 1090 Part 2”). See EN 1090.
  • AWS Inspection Trends, “Understanding Weld Cracking”; code wording quoted in AWS forum threads, tacks are fused into the root pass; cracked ones are removed; later passes do not remove a crack.
  • The site’s own pages, thin sheet, square tube, pipe and vertical-up tack sequences; distortion and the sequence of welding (thin sheet, distortion).

Frequently asked questions

How long should a tack weld be?

There is no single figure for every joint. For thin sheet the site gives a tack every 30–50 mm. In structural steelwork EN 1090-2 limits the tack length relative to the thickness, and the number comes from the edition in force. Short, flat and fused is the aim, not long.

How many tacks does a joint need?

Enough to hold the gap with the clamps and the sequence, and no more. Too few and the joint closes up as it cools; too many restrain it and invite cracks. Start in the middle and work outwards.

Do tacks have to be removed before welding?

Not if they are sound. A tack with tapered ends can be melted into the root run. A cracked tack, or one too large to melt through, is ground out.

Does a tack welder need a certificate?

The sources consulted do not settle it. If the tacks stay in a weld made to a standard, treat them as the weld and let a welder qualified for the joint put them in; the contract or the inspection body decides. See welder qualification.

Why do tacks crack?

A small tack cools very quickly, and on thick or hardenable steel it is hard and brittle. Apply the preheat of the WPS to tacks too and do not leave a cracked tack in the joint.

Where do tacks go on a pipe?

On the sides, not at 6 and 12 o’clock, where the halves start and close. Grind the ends to a taper and check the gap all round before tacking. See pipe welding positions.

Author: , welder and metal fabricator Updated: