Back purging: how to protect the weld root with gas
The arc gas protects the front of the weld. The back of the root, inside a tube or under a plate, sees air, and at welding temperature stainless steel, duplex, nickel alloys and titanium oxidise there within seconds. Back purging replaces that air with gas before the arc starts and keeps it there until the root has cooled.
Short answer
Close the cavity behind the root with dams or plugs, fill it with Ar or N₂+H₂ at 4–8 l/min, vent it at the far end and weld only when an oxygen meter at the vent shows the level the job asks for. For stainless where the root colour matters, about 50 ppm or lower is the usual target. Use argon for every metal; nitrogen–hydrogen forming gas only on austenitic stainless, never on titanium, duplex, ferritic or carbon steel. Keep the purge through the root and the hot pass. The colour tells you afterwards how well it worked: heat tint on stainless.
Why the root needs its own gas
Stainless steel resists corrosion because of a thin chromium oxide film. Heated in air, the surface grows a thick oxide instead, coloured from straw to blue and grey, and the metal just under it loses chromium. Inside an unpurged tube the root comes out black and granular: “sugaring”. That root is a corrosion site and often a crack starter, and on hygienic or chemical pipework it is cut out.
- Austenitic stainless (304L, 316L) — purge on tube, pipe and any joint whose back face is in service.
- Duplex and super-austenitic grades — purge always; the gas can contain nitrogen (see the table below).
- Nickel alloys — purge, as for stainless.
- Titanium and zirconium — purge, plus a trailing shield on the front: hot titanium takes up oxygen and nitrogen and becomes brittle. On titanium even a straw or purple colour means the shielding was not enough (TIG welding).
- Carbon and low-alloy steel — normally not purged. The root oxidises a little but keeps its properties.
Which colours are acceptable, and what AWS D18.1 allows inside tube: heat tint on stainless steel. Welding stainless in general: welding stainless steel.
Which purge gas: argon, forming gas, nitrogen
The site gas table gives Ar or N₂+H₂ for root purging at 4–8 l/min. Which one depends on the metal, not on what is at hand: a CO₂ welding mix is never used for purging.
| Gas | Used for | Not for |
|---|---|---|
| Argon (Ar) | All metals: stainless, duplex, nickel alloys, titanium, zirconium. TWI recommends pure argon as the backing gas. | — |
| Forming gas, nitrogen + hydrogen (N₂+H₂) | Austenitic stainless (304L, 316L). Hydrogen binds residual oxygen. | Carbon, ferritic, martensitic and duplex steels: hydrogen brings cracking and porosity. Titanium and zirconium. |
| Argon + nitrogen | Duplex and super-austenitic grades, per the WPS (TWI). | Titanium and zirconium. |
Hydrogen lightens the colour of the root, so a root purged with forming gas looks cleaner than one purged with argon at the same oxygen level. The colour charts were made with argon; judge a forming-gas root with that in mind. Mixtures with a higher hydrogen content are flammable: read the cylinder label and the safety data sheet, and vent to a safe place. In a closed room, tank or trench any purge gas displaces air: the oxygen meter at the vent does not protect the welder, room ventilation does (welding fume and ventilation).
Dams, plugs and venting
The smaller the space you have to fill, the faster and cheaper the purge. So the gas is held close to the joint instead of filling the whole pipe.
- Plugs and inflatable dams on both sides of the joint, joined by a hose: gas goes in through one, vents through the other. Common on pipe from small to large diameters.
- Water-soluble paper dams glued inside the tube, where a plug cannot be pulled out afterwards. They dissolve in the first water flush or pressure test.
- Tape over the joint gap (aluminium or purge tape) until the root run reaches it; peel it just ahead of the arc. An open gap lets air in and gas out.
- Plate and fittings: a channel, box or backing bar with gas holes behind the joint.
Always give the gas a way out. The vent should be about as large as the inlet; a blocked vent builds pressure that pushes the root bead inwards and leaves it concave, and TWI advises turning the pressure down slightly after the root so that the next pass does not blow through. Argon is heavier than air: feed it at the low point and vent at the high point. Nitrogen–hydrogen is lighter than air: feed high, vent low.

How long to purge: volume and gas exchanges
Purge time is set by the volume between the dams and the flow. One exchange (the flow has delivered as much gas as the cavity holds) does not remove all the air, because the gas mixes with it. Several exchanges are needed, and their number depends on the shape of the cavity, the leaks and the target. The table shows the starting point for the arithmetic, with the site flows of 4–8 l/min.
| Bore, mm | Length between dams, mm | Volume, l | One exchange at 4 l/min | One exchange at 8 l/min |
|---|---|---|---|---|
| 20 | 300 | 0.094 | 1.4 s | 0.7 s |
| 50 | 400 | 0.785 | 12 s | 5.9 s |
| 100 | 600 | 4.71 | 71 s | 35 s |
| 200 | 1 000 | 31.4 | 7.9 min | 3.9 min |
| 100 | 6 000 | 47.1 | 11.8 min | 5.9 min |
A 50 mm bore with dams 400 mm apart holds 0.79 l: one exchange takes about 6 s at the top flow. A 100 mm bore purged along a whole 6 m pipe holds 47 l, and one exchange there takes about 6 min. That is the case for dams. Turning the flow up does not save as much as it seems: a fast jet stirs the air into the gas instead of pushing it out. Find the bore of a standard tube in the steel pipe table. The purge ends when the meter at the vent reads the target, not when the clock says so.
Measuring residual oxygen
An oxygen meter (purge monitor) samples the gas at the vent or through a needle in the dam. The level the job needs is written in the specification or WPS. Two figures to orient by:
- About 50 ppm for stainless where the root colour matters. A purge equipment maker gives below 50 ppm for stainless steels, and on the AWS D18.2 chart 50 ppm is sample 3, the last one AWS D18.1 accepts as welded. 100 ppm is already sample 4 (heat tint chart).
- Titanium needs considerably less oxygen than stainless. Take the value from the procedure; published figures differ.
Measure after the gas has passed the joint, not at the cylinder. Purge gas also has to stay on while you weld: keep it through the root and the hot pass, and on thin wall or critical work through the first fill passes, as TWI advises. A root that is fine at the start and coloured further round usually means a leak opened as the joint heated, or the tape came off too early.
Gas consumption
A purge consumes gas for the whole time the joint is closed: the pre-purge, the welding, the pauses, the tack grinding. At 6 l/min, 30 minutes of plugged time is 180 l, however short the arc time. Enter the plugged time and the purge flow into the gas consumption calculator; the gas for the torch itself is chosen in the shielding gas selector and set by the TIG settings table. Dams pay for themselves here too: a smaller cavity needs a shorter pre-purge.
What goes wrong
- Black, granular root (“sugaring”). No purge or the purge failed: leak, open gap, too short a pre-purge. Cut out and reweld.
- Blue or brown root despite purging. The oxygen is still too high or moisture is in the cavity: purge longer, check hoses and connections, dry the parts. Judge the colour by the heat tint chart.
- Concave or sunken root. Too much purge pressure or a blocked vent; see lack of penetration for the other root faults.
- Colour only at the end of the seam. The tape was removed too far ahead, or the dam moved.
- Porosity at the root. Wet dams or a damp cavity, a CO₂ mix used for purging, or turbulence from too high a flow (porosity).
Standards and references
Where the figures on this page come from. AWS D18.1/D18.2 are cited through published papers, as on the heat tint page; the full standard texts were not consulted.
- TWI, FAQ: heat tint during welding of stainless steels, control of oxygen before welding, pure argon, argon–nitrogen for duplex, purge through the root and hot pass, less pressure after the root.
- Huntingdon Fusion Techniques, “Purging in welding”, oxygen below 50 ppm for stainless steels.
- AWS D18.2 / D18.1 (papers at the 3-A SSI annual meeting, 2016), 50 ppm = sample 3, 100 ppm = sample 4: heat tint on stainless.
- This site: gas table and gas pages, purge flow 4–8 l/min, Ar or N₂+H₂; hydrogen only on austenitic stainless: shielding gas selector, TIG welding.
Frequently asked questions
What is back purging in welding?
Filling the space behind the root (the inside of a tube or the area under a plate) with inert gas, so that the hot root does not oxidise. It is used on stainless steel, duplex, nickel alloys and titanium. The gas is held between dams or plugs and vented at the far end.
Can I use forming gas instead of argon?
On austenitic stainless such as 304L and 316L, yes: nitrogen–hydrogen is a common purge gas there. Not on titanium, duplex, ferritic, martensitic or carbon steel, where hydrogen causes cracking and porosity. Argon works on every metal.
How long should I purge before welding?
Until an oxygen meter at the vent shows the target, not for a fixed time. The time grows with the volume: a 50 mm bore between dams 400 mm apart holds 0.79 l, a whole 6 m pipe of 100 mm bore holds 47 l. Dams close to the joint cut the purge time.
What oxygen level do I need for stainless?
The specification decides. Where the root colour matters, about 50 ppm or lower: that is sample 3 on the AWS D18.2 chart, the last one AWS D18.1 accepts as welded, and the figure a purge equipment maker gives for stainless.
What purge flow rate should I use?
The site gas table gives 4–8 l/min. A higher flow is not much faster: it stirs the air into the gas. After the root, turn the pressure down a little so the next pass does not push the root in.
Does carbon steel need a back purge?
Normally not. The root of carbon and low-alloy steel oxidises slightly but keeps its strength. Purging is for stainless, duplex, nickel alloys and titanium.
Updated: