How to weld wear-resistant and quenched and tempered steel
Wear plate (hardness classes around 400 and 500 HB) and quenched and tempered structural steel such as S690QL get their properties from heat treatment at the mill. Welding heats them again. Too fast a cooling plus hydrogen gives cold cracks; too much heat softens the heat-affected zone, and the plate loses there the hardness or strength it was bought for.
Short answer
Work out the preheat from the plate CET, the thickness and the hydrogen level, weld with low-hydrogen (H5) consumables, and stay below the maximum interpass temperature on the steel data sheet. On wear plate the filler is usually weaker than the plate: unalloyed or low-alloyed, or austenitic (307 or 309 type), which tolerates hydrogen and on most grades needs no preheat. Keep the heat input in the window the steel maker gives. The numbers: preheat calculator, carbon equivalent, cooling time t8/5.
Why these steels are harder to weld
The plate has been hardened by quenching and, for most grades, tempered afterwards. That structure is good for wear and strength, and the welding cycle disturbs it in two ways.
- Cold (hydrogen) cracking. The steel is hardenable, so the heat-affected zone next to the fusion line can harden on cooling. With diffusible hydrogen and the stress of the joint, cracks form, sometimes hours after welding. The three conditions and how to remove them are on the steel weldability page; the cure here is preheat, dry low-hydrogen consumables and an even sequence.
- Softening of the heat-affected zone. Where the weld heats the plate above its tempering temperature, the quench-and-temper effect is lost. A band next to the weld becomes softer than the plate: on wear plate it wears faster, on S690QL it is weaker. The more heat and the hotter the interpass, the wider the band.
So the window is narrow from both sides: too cold gives cracks, too hot gives a soft zone. Group 3 in ISO/TR 15608 covers the quenched and tempered steels; post-weld heat treatment for them is only applied by procedure and below the tempering temperature, and ordinary wear plate is normally not heat treated after welding.
CEV and CET: read them from the certificate
Two carbon equivalents are used. CEV (the IIW formula, CE = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15) says how awkward the steel is; CET = C + (Mn+Mo)/10 + (Cr+Cu)/20 + Ni/40 is the input for preheat by EN 1011-2 method B. Both are computed from the heat analysis, and both rise with plate thickness on wear and Q&T grades, because thicker plate needs more alloy to harden through. Take them from the inspection certificate or the maker’s data sheet for that thickness; do not use a “typical” value for another thickness.
The carbon equivalent calculator computes CE from the analysis. S690QL (1.8928, close to ASTM A514 Gr. B) is listed in the steel grade equivalents.
Preheat: by CET, thickness and hydrogen
The table is computed by the same formula as the preheat calculator (EN 1011-2, annex C, method B) at a heat input of 1.5 kJ/mm. The CET values are examples, not the values of any particular grade: put in the CET from your certificate.
| Thickness, mm | CET 0.35 · HD 5, °C | CET 0.40 · HD 5, °C | CET 0.45 · HD 5, °C | CET 0.40 · HD 10, °C |
|---|---|---|---|---|
| 10 | 50 | 90 | 130 | 120 |
| 15 | 70 | 110 | 150 | 140 |
| 20 | 90 | 130 | 165 | 160 |
| 30 | 120 | 155 | 195 | 185 |
| 40 | 140 | 175 | 215 | 205 |
| 60 | 155 | 195 | 235 | 225 |
Heat input 1.5 kJ/mm, rounded up to 5 °C as in the calculator; “—” means the formula asks for no preheat. HD 5 corresponds to H5 consumables. The method applies to CET 0.20–0.50 and 10–90 mm; the steel maker’s data take precedence.
Three things to read from it. At CET 0.40 and 20 mm the formula gives 130 °C with H5 consumables and 160 °C at HD 10, more than H5 needs at 30 mm (155 °C): in this example hydrogen weighs more than 10 mm of extra plate. Thickness matters up to about 40 mm (175 °C) and less after that. And at CET 0.45 and 60 mm the result, 235 °C, is above the 200 °C the pWPS generator puts as the interpass maximum for group 3.1: when the preheat approaches the maximum, the job needs another approach, for example an austenitic filler or the maker’s procedure. Steel makers also publish their own preheat tables by grade and thickness (often for the combined thickness of the joint); where these exist, they govern. In a joint of two different plates, the plate that needs the higher preheat decides.
Filler: why weaker than the plate is often right
The weld metal of a wear plate is never as hard as the plate, whatever the filler. What the filler can do is resist cracking. So on wear plate the usual choice is a filler weaker than the plate: it is tougher and tolerates hydrogen better, which lowers the risk of cracks. On S690QL in a load-bearing joint the designer sets the strength, and the filler may have to match.
| Filler type | Examples of designation | When |
|---|---|---|
| Unalloyed or low-alloyed, below the plate strength | MAG wire G 42 / G 46 (EN ISO 14341), electrode E 42 / E 46 … H5 (EN ISO 2560) | The usual choice on wear plate: tougher weld metal, lower cracking risk. Preheat by the calculator. |
| Austenitic stainless | 18 8 Mn (AWS 307 type), 23 12 L (309L type) | Wear plate where preheat is hard to apply, repairs, joints to other steels. Tolerates hydrogen; on most grades no preheat needed. |
| Matching high-strength | G 69 (EN ISO 16834), E 69 … H5 (EN ISO 18275) | S690QL in load-bearing joints where the design needs the full strength. Strict preheat, heat input and hydrogen control. |
Whatever the type, keep the hydrogen at H5 or below: basic electrodes baked and kept warm per the maker, flux-cored wire kept dry, packs opened just before use. Baking temperatures by electrode type: electrode drying table. Where the weld surface itself is in the wear path, the joint is capped with a hardfacing deposit; the joint underneath stays as described here.
Interpass temperature and heat input
The interpass temperature has a minimum (the preheat) and a maximum. For quenched and tempered steels the maximum protects the heat-affected zone from softening; the pWPS generator uses 200 °C for group 3.1 as a starting value, and the steel data sheet gives the exact value for each grade and thickness: take that one. How to measure: interpass temperature.
The heat input is the other half. Too low, and the zone cools fast and hardens; too high, and it softens and loses toughness. For S355 the usual t8/5 window is 5–25 s; for Q&T steels the maker gives its own, narrower range. Check the run with the heat input calculator and the t8/5 calculator. In practice: stringer beads rather than wide weaves, several small runs instead of one large one, and a thermometer or temperature crayon between runs.

Order of work
- Find the grade, thickness and CET (certificate or data sheet).
- Choose the filler: weaker unalloyed or low-alloyed, austenitic, or matching where the design needs it, all H5 or better.
- Calculate the preheat; check it against the maker’s table and the interpass maximum.
- Clean and dry the joint; preheat a band on both sides and check the temperature on the side away from the heat source.
- Weld in stringer beads, checking the interpass temperature.
- Let the joint cool slowly in still air; no water, no compressed air.
- Inspect for cracks after cooling, and on critical parts again later, because hydrogen cracks can be delayed (weld cracks).
Write it into the WPS, with preheat and interpass as separate lines: welding procedure specification.
Standards and references
Where the figures and rules on this page come from. EN 1011-2 is applied through the site calculators; the full standard text was not consulted. Brand names are examples of the class only.
- SSAB, How to weld (ssab.com), hydrogen max 5 ml/100 g, lower-strength and austenitic (307, 309) consumables, preheat by grade and thickness, the plate with the higher preheat decides, maximum temperatures from the data sheet.
- EN 1011-2, annex C, method B (as in the site calculator), preheat from CET, thickness, hydrogen and heat input: preheat calculator.
- EN ISO 2560, EN ISO 14341, EN ISO 16834, EN ISO 18275, filler designations; H5 = no more than 5 ml/100 g.
- This site: pWPS generator, t8/5 and interpass pages, 200 °C for group 3.1, t8/5 window: pWPS, t8/5, interpass temperature.
Frequently asked questions
Do you need to preheat wear plate before welding?
Usually from a certain thickness, and the threshold falls as the hardness class rises. Calculate it from the CET, the thickness and the hydrogen level (preheat calculator) and compare with the steel maker’s table. With an austenitic filler most grades can be welded without preheat.
What filler do you use on HB400 wear plate?
Usually a low-hydrogen (H5) unalloyed or low-alloyed wire or electrode that is weaker than the plate, for example G 42 or E 42 class, or an austenitic 307 or 309 type. The weld will not be as hard as the plate with any filler; the aim is a joint that does not crack.
Why does the area next to the weld wear faster?
The heat of welding tempers the quenched plate next to the weld and it softens. Less heat input and a lower interpass temperature keep that band narrow. If the weld itself is in the wear path, a hardfacing cap protects it.
What is the maximum interpass temperature for Q&T steel?
It is given on the steel data sheet for each grade and thickness. The site pWPS generator uses 200 °C for group 3.1 (S690Q and similar) as a starting value. Exceeding it softens the heat-affected zone.
Can wear plate be stress relieved after welding?
Ordinary wear plate is normally not: heating it would take away the hardness. For quenched and tempered structural steel, post-weld heat treatment is applied only by procedure, below the tempering temperature: PWHT.
Why do cracks appear hours after welding?
Hydrogen cracks are delayed: hydrogen diffuses to the hard zone and the crack opens later. That is why the inspection on these steels is done after the joint has cooled, and on critical parts again later. Prevention: preheat, H5 consumables, dry joint.
Updated: