Sections

Site map →

EN

How to weld copper and brass

Copper pulls heat out of the weld zone faster than any common structural metal, and it is picky about its own oxygen content. Brass adds a second problem: zinc boils at 907 °C, below the temperature of the pool, and leaves as fume.

Short answer

Choose the grade first: deoxidised Cu-DHP welds, tough-pitch Cu-ETP does not. Weld with TIG on DC− (argon on thin material, helium or an Ar–He mixture as thickness grows) or with MIG on thicker work. A silicon bronze filler, CuSi3 (S Cu 6560), is the usual all-round choice for copper and brass. Thin material usually needs no preheat; thick material needs it, about 250 °C for MIG on heavy sections. On brass keep the heat low and the fume extracted: welding fume and ventilation.

Why copper is hard to weld

Cu-ETP conducts about 394 W/(m·K) at 20 °C, deoxidised Cu-DHP about 305 W/(m·K), and both figures are many times those of steel. The arc heats the spot, the plate carries the heat away and the pool does not form until the surrounding metal has warmed up. Three consequences follow.

  • Lack of fusion at the start and on thick sections. A cold start leaves the first centimetres unfused unless you raise the current or preheat. TWI says preheat is needed on thick sections.
  • Distortion. Copper expands strongly; TWI notes that the root gap can close as the joint heats, so the gap is set with that in mind (welding distortion).
  • Soft heat-affected zone. Heat cannot harden copper, and it softens cold-worked copper, so a joint is weaker than the rolled or drawn material.

The weight of the workpiece tells you how much metal there is to heat: see the copper weight calculator and the brass weight calculator.

Advertisement

Cu-DHP, Cu-ETP, oxygen-free: which welds and why

Copper comes in three grades that matter here.

  • Cu-ETP (tough pitch, CW004A). Contains oxygen as copper oxide. In the weld the oxide breaks down and, with hydrogen present, forms steam that blows pores and opens cracks along the grain boundaries. This is hydrogen disease. It also happens in a reducing (excess acetylene) flame, because hydrogen from the flame diffuses into the hot metal.
  • Cu-DHP (phosphorus-deoxidised, CW024A). The phosphorus has taken up the oxygen, so there is no hydrogen disease. This is the grade of tube and parts made for welding and brazing. Porosity is still possible, especially without filler, so use a filler with deoxidants.
  • Oxygen-free copper. The most weldable, the choice for electrical and vacuum work.

The grade is printed on the material certificate or tube marking. If it is not known, treat the copper as Cu-ETP: use a deoxidising filler, avoid the autogenous weld and keep a reducing flame out of it. The three grades weigh the same to within 0.3 %, which is why the weight calculators treat them alike.

Processes: TIG, MIG, gas

  • TIG, DC−. The standard process for tube, thin sheet and repairs. Copper is welded on DC−, like steel and stainless (the TIG page has the polarity table). Argon covers thin material, helium or an argon–helium mixture raises the heat from a few millimetres up. Argon at 6–10 l/min is the starting flow from the site gas table; helium needs more. Tungsten and current: tungsten colour codes and the tungsten calculator.
  • MIG. For thick sections: it puts in more heat than TIG and welds faster. Argon, or argon with helium on heavy work. A wire feed that is smooth matters because copper-based wires are soft (wire feeding problems).
  • Gas welding works on deoxidised Cu-DHP with a neutral flame, for example on plumbing tube; see gas welding. Not on Cu-ETP in a reducing flame.
  • MIG brazing (braze welding) with CuSi3 does not melt the copper: next sections.

Copper to copper is welded; copper to steel is better brazed or braze-welded, with the steel side taking most of the heat (dissimilar metals).

Filler wires and rods: the designations

The designations below come from ISO 24373 (copper and copper-alloy filler for arc welding). The older names in the right column are the ones still printed on many spools and rods.

Copper filler metals, ISO 24373
ISO 24373AlloyUsed for
S Cu 6560CuSi3Mn1 (silicon bronze, about 3 % Si, 1 % Mn)Copper, brass, braze welding of thin sheet and of copper to steel; also overlay on steel. The usual all-round choice.
S Cu 1898CuSn1 (about 1 % tin)Copper and low-alloyed copper; more fluid on thin material.
S Cu 1897CuAg1 (about 1 % silver)Oxygen-free copper where conductivity matters; not for oxygen-bearing copper.

The first choice for most copper work is S Cu 6560: silicon and manganese deoxidise the pool, and TWI names the equivalent ERCuSi-A as the preferred filler for tough-pitch and phosphorus-deoxidised copper. The tin wire flows easily on thin material. CuAg1 keeps the electrical conductivity high and is for oxygen-free copper; the makers’ data sheets say it is not for copper that contains oxygen. Match the rod to the work in the WPS (welding procedure specification).

Brass: zinc evaporates

Brass is copper with zinc, 37 to 40 % in the common grades (CuZn37, CuZn40; their weights are in the brass calculator). Zinc boils at 907 °C, well below the temperature of the weld pool, so it leaves as white zinc oxide fume and leaves pores behind. The consequences are the same as on galvanized steel:

  • Fume. Zinc oxide causes metal fume fever: fever, chills and a metallic taste hours after the shift. Extraction at the arc first, then a respirator in a confined space (welding fume and ventilation, respirators).
  • Pores. The weld metal loses zinc and boils; the weld ends up with a different composition from the base metal.
  • Fusion welding with a brass rod makes the most fume. A CuSi3 or tin-bronze rod has no zinc in it, so only the base metal gives off zinc, and the heat input can be kept lower.

Braze welding with CuSi3

In braze welding the filler melts and the base metal does not, or only at the surface: a CuSi3 wire melts at a lower temperature than copper or steel, wets the joint and fills it. This is why CuSi3 is used on thin brass sheet, on thin galvanized sheet (less burning of the zinc coating, less spatter) and on copper-to-steel joints. The joint is weaker than a fusion weld in thick copper and has a different colour, so it is not used where the specification asks for a fusion weld or a colour match.

  • Gas: argon, TIG or MIG.
  • Heat: low current, small pool, fast travel: just enough for the wire to wet the surface.
  • Clean metal: brush or abrade the oxide off immediately before.

Material → process → filler → preheat

Starting points for the WPS. Thicknesses are not given as exact limits because the sources differ; the temperature of 250 °C is the one both sources confirm.

Welding copper and brass: material, process, filler, preheat
MaterialProcess and gasFillerPreheat
Cu-DHP, thin sheet and tubeTIG, DC−, argonS Cu 1898 (CuSn1) or S Cu 6560 (CuSi3Mn1)Usually none; rises with thickness
Cu-DHP, thickTIG with helium or Ar–He, or MIG with argon / Ar–HeS Cu 6560, S Cu 1898Yes; about 250 °C for MIG on heavy sections
Cu-ETPTIG, DC−, argon, deoxidising filler; no autogenous weld, never a reducing flame; the heat-affected zone can embrittleS Cu 6560 (CuSi3Mn1)As Cu-DHP of the same thickness
Oxygen-free copperTIG, DC−, argon or Ar–HeS Cu 1897 (CuAg1), S Cu 1898As Cu-DHP of the same thickness
Brass CuZn37, CuZn40TIG or MIG braze welding, argon; low heat, extractionS Cu 6560 (CuSi3Mn1), S Cu 1898Little or none; set by the WPS
Copper or brass to steelMIG or TIG braze welding, argon, aim the arc at the copper sideS Cu 6560 (CuSi3Mn1)Per the WPS; the copper side takes the heat (dissimilar metals)

Preheat above about 250 °C and currents above about 350 A call for heat shields and for thought about the welder’s health, according to TWI.

Typical faults on copper and brass

  • Pores in the weld. Oxygen-bearing copper (hydrogen disease), no deoxidising filler, damp or oily metal, wrong gas. See porosity in welds.
  • Cracks along the grain boundaries on Cu-ETP in a reducing flame or with hydrogen: change the grade, use a filler with Si and Mn (weld cracks).
  • Lack of fusion at the start and root. Not enough heat for the plate that carries it away: higher current, helium, preheat, a hot start.
  • Dark, dull weld. Gas flow or post-flow too short: the hot copper oxidises before it cools.
  • White deposit and smoke on brass. Zinc oxide: reduce the heat or change to CuSi3.

Standards and references

Where the figures on this page come from. ISO 24373 is cited through the filler makers’ data sheets; the full standard text was not consulted.

  • TWI, Job Knowledge: Welding of copper and its alloys (part 1), grades and oxygen, hydrogen porosity, ERCuSi-A, gases by thickness, preheat on thick sections and for MIG, shields above 250 °C.
  • Filler data sheet CuSi3 (MT-CuSi 3, 2.1461, DIN 1733), no preheat for TIG, about 250 °C for MIG on thick work, use on copper and brass.
  • ISO 24373 (via data sheets of Castolin, Magmaweld, Gedik, GYS), S Cu 6560 (CuSi3Mn1), S Cu 1898 (CuSn1), S Cu 1897 (CuAg1); CuAg1 for oxygen-free copper only.
  • Material data sheets Cu-ETP CW004A (Metalxact, Schlenk) and Cu-DHP CW024A (Bikar, Metalxact), thermal conductivity 394 and 305 W/(m·K) at 20 °C.
  • Los Alamos National Laboratory; American Galvanizers Association, zinc boils at 907 °C (as on the galvanized steel page).
  • This site: polarity and gas tables, DC− for copper, argon flow for TIG: TIG welding.

Frequently asked questions

Can you weld copper with a MIG welder?

Yes. MIG welds thick copper faster than TIG and puts in more heat. Use argon, or argon with helium on heavy sections, and preheat thick work: about 250 °C on heavy sections. For thin copper and tube TIG is easier to control.

What polarity do you use to TIG weld copper?

DC−, electrode negative, like steel and stainless. AC is for aluminium and magnesium. Pick the tungsten from the colour table.

Why does copper crack or go porous when welded?

The usual cause is oxygen in the copper: tough-pitch Cu-ETP forms steam in the weld when hydrogen is present, which gives pores and grain-boundary cracks (hydrogen disease). Use deoxidised Cu-DHP or oxygen-free copper, a filler with silicon and manganese, and no reducing flame.

What is CuSi3 and what is it used for?

CuSi3 is a silicon bronze filler, S Cu 6560 (CuSi3Mn1) in ISO 24373. It welds copper and brass and is used for braze welding thin sheet, galvanized sheet and copper-to-steel joints with less heat than a fusion weld.

Is brass welding dangerous?

The zinc in brass boils at 907 °C and leaves as zinc oxide fume, which causes metal fume fever. Extract at the arc, add a respirator in a confined space and keep the heat low: welding fume and ventilation.

Does copper need preheating?

Thin copper and tube usually do not. Thick sections do, because the metal carries the heat away: about 250 °C is quoted for MIG on heavy sections, and the temperature rises with thickness. The value for your job goes in the WPS.

Author: , welder and metal fabricator Updated: