Slag inclusions (301): where they come from and how to stop them
A slag inclusion is slag from the coating, the flux core or the flux that the next run buried instead of melting out. It forms at three places: on a run that was not cleaned, in a notch at the toe of the run below, and in front of an arc that let the slag run ahead of it.
Short answer
Slag inclusions (ISO 6520-1 no. 301) come from processes that make slag: stick (111), flux-cored wire (136, 114) and submerged arc (121). Clean every run down to bright metal along the toes, grind out notches and humped beads before the next run, keep the arc ahead of the slag, give the electrode room in the groove (60° for stick) and stay inside the current range for the diameter (3.2 mm: 90–140 A). Between runs they are found by eye; once buried, by radiography (RT). A dark line along the side wall is often lack of fusion with slag in it (4012), which no quality level permits.
What counts as a slag inclusion
ISO 6520-1 puts it in group 3, solid inclusions. The numbers you will meet on a report:
- 301 slag inclusion, with 3011 linear (a line, usually along a side wall or between runs), 3012 isolated (a single irregular piece) and 3013 clustered;
- 302 flux inclusion, the same thing from submerged arc flux;
- 4012 lack of inter-run fusion, which on a film or a section often carries slag with it and is mistaken for 3011.
The full list and the other groups are in the ISO 6520-1 imperfection table; the short cause-and-remedy overview of all groups is in the weld defect catalogue.
Solid-wire MAG (135) and TIG (141) make no slag blanket, so 301 is rare there. Metal-cored wire (138) leaves practically no slag either. With stick, flux-cored wire and submerged arc the slag is part of the process: it shields and shapes the bead, and it has to come off after every run.
Causes, signs and what to change
Most slag inclusions can be traced to one of these. The first two account for the bulk of multi-run work.

| Cause | Typical sign | What to change |
|---|---|---|
| Previous run not cleaned | Isolated or linear slag between runs; on the film, pieces at the level of an interface between runs | Chip and wire-brush every run down to bright metal, toes included. With 136 and 114 after every run. |
| Notch at the toe of the previous run (undercut, humped bead, deep corner between beads) | A slag line along one side wall or between two fill runs (3011) | Grind the hump and the undercut before the next run; place runs so they wet both sides. |
| Slag running ahead of the arc | Slag under the run, often at the start of a downhill section or with a slow travel speed | Increase travel speed, reduce the lean of the electrode, drag flux-cored wire instead of pushing it. |
| Groove too narrow for the process | Slag lines at both side walls, often with lack of side-wall fusion | Open the groove: 60° for stick, 50–60° for MAG, or use a smaller electrode for the root and the first fill runs. |
| Current too low, arc too long | Slag and lack of fusion together; a convex, poorly wetted run | Current in the range for the diameter (3.2 mm: 90–140 A flat), a short arc. |
| Stops, restarts and tacks not cleaned | Single slag pieces at regular intervals, at the tie-ins | Grind craters and tack ends to a taper and clean them before welding over. |
| Root not cleaned before the hot pass, or slag in the root edges | Two parallel lines at the root edges on the film | Grind the root face side of the root run clean; run the hot pass hot enough to melt the edges. |
Lack of fusion and slag often appear together: a cold run does not melt the slag out and does not melt the side wall either. The fusion side is covered on lack of fusion.
Stick, flux-cored and submerged arc: what differs
- Stick (111). Every run leaves a slag crust. Rutile slag lifts by itself; basic slag is dense and has to be chipped between runs, and it holds hardest in a narrow groove and at the toes. The groove is opened wider for stick (60°) than for MAG (50–60°), because the coated electrode needs room to reach the bottom and the slag has to be chipped out. Electrodes and their coatings: coating types.
- Flux-cored wire (136, 114). The torch is dragged so that the slag stays behind the pool; pushing it, as with solid wire, drives the slag in front of the arc. Deslag after every run with a hammer and a wire brush along the toes. Details on flux-cored arc welding.
- Submerged arc (121). The slag usually lifts off by itself on a well-shaped run; it is trapped where a run is placed too close to the side wall or onto a humped run below. Recycled flux is sieved free of dust and slag. More on submerged arc welding.
How to find it: between runs and after welding
- Visual inspection between runs is the cheapest check and the only one that prevents the defect. After deslagging look along both toes with a light at a low angle: grey or glassy spots in the corner, a groove the hammer did not reach, an undercut at the side wall. Clean or grind them before the next run.
- Radiography (RT) shows slag as dark, irregular shapes: single pieces, lines along one or both side walls, or two parallel lines at the root edges. RT is the method for volumetric imperfections such as pores and inclusions, and it leaves a record image.
- Ultrasonic testing (UT) finds slag lines too, but it is the stronger method for planar flaws such as lack of fusion, which matters because the two are often found together.
- Macro section on a test piece shows where the slag sits: between runs, at a side wall or at the root.
Which method applies to which joint, and which standard sets the acceptance levels, is on NDT of welds: ISO 10675-1 for radiographic indications in steel, ISO 11666 for ultrasonic indications.
Quality levels: how much ISO 5817 allows
ISO 5817 has its own row for solid inclusions (300) with a limit for each of the levels B, C and D, level B being the strictest. The limit table on this site does not carry that row yet, so take the figure from the standard itself or from the acceptance criteria in your contract or WPS. What the site table does give is the neighbours that slag is confused with:
| No. | Imperfection | B — stringent | C — intermediate | D — moderate |
|---|---|---|---|---|
| 2011 | Isolated gas pore | 0.2·t max 3 mm | 0.3·t max 4 mm | 0.4·t max 5 mm |
| 401 | Lack of fusion | not permitted | not permitted | not permitted |
| 4021 | Incomplete penetration (lack of root penetration) | not permitted | not permitted | 0.2·t max 2 mm (short imperfections only) |
The practical consequence: an indication that is a line along the side wall is not judged as a slag inclusion if it turns out to be lack of fusion (401, 4012), because lack of fusion is not permitted at any level. Other thicknesses and the other imperfections: ISO 5817 limits calculator and quality levels B, C, D.
Repair: cut out and weld again
- Locate it: position along the weld from the film or the UT report, depth from UT. Mark both ends on the part.
- Remove it by grinding or gouging until the slag is gone and the walls are bright metal. Shape the excavation like a small U groove with a rounded bottom, so the electrode reaches the bottom and the new slag can be cleaned out.
- Check the excavation visually, and with PT or MT if the job asks for it, before welding.
- Weld to the procedure of the joint, cleaning every run, with the preheat and interpass temperature the procedure gives.
- Inspect again with the same method that found the defect.
The general repair sequence, including preheat for crack repairs, is on repair welding.
Prevention checklist for multi-run welds
- Chip and wire-brush every run, including the tacks, starts and craters; grind where the hammer does not reach.
- Aim for a flat or slightly concave run that wets both sides. A humped run with deep corners beside it is the classic slag trap: grind it flat before the next run.
- Grind out undercut at the side wall before covering it.
- Place each fill run so that it melts into the side wall and the previous run, not into the corner between them.
- Keep the arc ahead of the slag: a travel speed that is too slow, or an electrode that leans too far, lets the slag run under the arc, especially downhill.
- Stay inside the current range for the electrode diameter: 2.5 mm 70–100 A, 3.2 mm 90–140 A, 4.0 mm 130–190 A in the flat position (site table; less in position). A cold pool freezes before the slag floats out. The current calculator adds the position and coating.
- Open the groove wide enough for the process: groove calculator.
Standards and sources
This page adds no figures of its own. The numbers come from the tables of this site.
- ISO 6520-1, imperfection numbers 301, 3011, 3012, 3013, 302 and 4012, as in the ISO 6520-1 table.
- ISO 5817, the limits for 2011, 401 and 4021 from the site table on quality levels B, C, D; the row for solid inclusions (300) is not reproduced.
- ISO 9692-1, included angle by process, as in the groove calculator.
- ISO 10675-1, ISO 11666, acceptance levels for radiographic and ultrasonic indications, as listed on NDT of welds.
Frequently asked questions
What causes slag inclusions in a weld?
Mostly slag left on the previous run, and notches at its toes (undercut, a humped bead) that the hammer cannot reach. Then slag running ahead of the arc, a groove too narrow for the electrode and a current too low for the slag to float out.
How do I tell slag from lack of fusion on a radiograph?
Slag gives an irregular dark shape; lack of fusion along a side wall gives a thin straight line, often with slag in it. When in doubt, UT or a macro section on a test piece decides. The difference matters: lack of fusion is not permitted at any ISO 5817 level.
Can MIG or TIG welding give slag inclusions?
Rarely. Solid-wire MAG (135) and TIG (141) make no slag blanket, and metal-cored wire (138) leaves practically none. Slag inclusions belong to stick, flux-cored wire and submerged arc. Solid-wire MAG leaves only spatter and a thin glassy film; brush the film off before the next run.
How much slag inclusion does ISO 5817 allow?
ISO 5817 sets a limit for solid inclusions (300) at each of the levels B, C and D, strictest at B. This site’s limit table does not carry that row, so take the figure from the standard or from your acceptance criteria; RT acceptance levels are in ISO 10675-1.
Is a slag inclusion repaired or can it stay?
If it is within the acceptance level, it can stay. If not, it is ground or gouged out to bright metal, the excavation is checked, rewelded to the procedure and inspected again with the same method.
Why does slag collect along the side walls?
The corner between a fill run and the groove wall is the last place the hammer reaches, and a humped run or an undercut deepens it. Grind those before the next run and place the runs so they melt into the wall.