How to weld an open root: gap, root face, keyhole and the back side
The root run is the one weld in a joint that has to fuse both root faces and form a bead on the side you cannot see. Fit-up decides most of it before the arc is struck: gap, root face and how the tacks hold them.
Short answer
For a single-V up to 12 mm: root face 1–2 mm, gap 2–4 mm for stick and TIG, 1–3 mm for MAG, measured after tacking. Root with an electrode a size smaller than the fill (3.2 mm: 90–140 A flat, 75–120 A vertical, 70–110 A overhead), and keep a small keyhole open at the front of the pool: both root faces melting into it, the same size all the way. If it closes, there is no penetration; if it grows, burn-through is next. Then check the back side before the next run.
Gap and root face before you strike
The figures below are the site’s groove table (ISO 9692-1 typical values, the same as the groove calculator). The WPS has the final say where there is one.
| Joint and process | Included angle α | Gap b | Root face c |
|---|---|---|---|
| Single-V, 3–12 mm, stick (111) | 60° | 2–4 mm | 1–2 mm |
| Single-V, 3–12 mm, MAG (135) | 50–60° | 1–3 mm | 1–2 mm |
| Single-V, 3–12 mm, TIG (141) | 60–70° | 2–4 mm | 1–2 mm |
| Double-V (X), 12–40 mm | 60° (MAG 50–60°) | 1–3 mm | 1–3 mm |
| Square edge (I), up to 3 mm (MAG up to 4 mm) | — | 0–2 mm up to 2 mm thick, 1–3 mm above | — |
- Root face is what stops the root from burning away. Measure it at both ends and in the middle: a hand-ground or flame-cut edge that wanders gives a root that alternates between burn-through and lack of penetration.
- Gap is what lets the arc down to the bottom. Set it with spacers and re-measure after every tack, because each tack shrinks and pulls the gap closed. Size and spacing of tacks: tack welds.
- Edges level. Misalignment (hi-lo) leaves one root face higher than the other, and the arc fuses only the near one.
- Grind tack ends to a taper so the root runs into them without an unfused spot. Cutting and cleaning the bevel: joint preparation.
Electrode, current and process
Stick (111). The root is usually one electrode size smaller than the fill, so that the tip reaches the root face. Starting ranges from the site’s current table, reduced for position:
| Electrode, mm | Flat (PA), A | Vertical up (PF), A | Overhead (PE), A |
|---|---|---|---|
| 2.5 | 70–100 | 60–85 | 55–80 |
| 3.2 | 90–140 | 75–120 | 70–110 |
- Set the current on a scrap piece with the same gap and root face. Too hot and the keyhole grows and the bead sags through; too cold and the root faces stay unfused. The current calculator adds coating and position.
- MAG (135). The root runs in dip transfer into an open gap; the high currents in the MAG table are fill figures. Settings: MIG/MAG settings.
- TIG (141). The best-controlled root and the usual choice on pipe and on stainless, with stick or wire for the fill. Add the wire at the leading edge of the keyhole. Tungsten and current by thickness: TIG settings.
The keyhole: how to run the root
- Strike on the tack or in the groove just ahead of it, and let the pool fuse into the tack end.
- Open the keyhole: hold the arc at the bottom of the groove until a small hole forms at the front of the pool with both root faces melting into it.
- Travel at the speed that keeps it one size. A pool about twice the gap wide fuses both faces; with a 3 mm gap that is roughly 6 mm.
- If the keyhole closes, slow down, shorten the arc and check the gap ahead. No keyhole on an open root means no penetration.
- If it grows, speed up, flick the arc forward onto the root faces for a moment, or reduce the current. A keyhole that keeps growing ends in burn-through.
- Keep the arc short and on the root, not on the bevels: an arc burning on the bevel walls bridges over the gap and leaves the bottom unfused.

On fixed pipe the position changes around the joint, and so does the current: the band is lowest at the bottom (overhead). Positions and the order of welding around the pipe: pipe welding positions.
Stops, restarts and tie-ins
- Before you stop, move the arc back onto the finished bead or onto the bevel so that the crater does not sit in the keyhole.
- Grind every stop and every tack end to a taper before you weld into it. A blunt end leaves an unfused spot or a pocket of slag under the restart.
- Restart a little behind the crater, re-open the keyhole and only then move on.
- On pipe, finish each half on the ground-down end of the other one, not on a fresh crater.
Backing and gas on the root side
Where the back side is out of reach, or the root must be formed reliably, the pool is held or protected from below.
| Backing | What it does | Watch out for |
|---|---|---|
| Ceramic tiles on adhesive tape | Shape a smooth root bead; come off after welding | Tape and tile must sit tight along the whole gap |
| Copper bar | The weld does not stick to it; its groove shapes the root | Where it stands off the joint, the pool drops through |
| Permanent steel strip or ring | Becomes part of the joint; the root is fused into it | Both root faces and the backing must fuse; the notch it leaves is a design decision |
| Consumable insert | A ring or strip of filler placed in the joint and melted into the root | Used on pipe to a qualified procedure |
| Argon purge (no solid backing) | Keeps air off the hot root of stainless and other alloys | Without it the back of a stainless root oxidises into a rough, crumbly crust |
Gas protection of the root side (back purging) is its own subject: how to seal the pipe, flow and when the oxygen is low enough to strike. See back purging and, for what an oxidised stainless root looks like, heat tint on stainless and welding stainless steel.
Check the back side before the next run
- Where you can see it: a continuous bead through the whole length, both root edges fused into the parent metal, a slight reinforcement, no holes and no hollow.
- On pipe and closed sections use a mirror at an open end, or an endoscope through an opening. That is the quickest check before the fill.
- From the top: clean the root run, grind humps and the slag lines at its edges, check that the tie-ins are smooth. Then the second run (hot pass) goes in hot enough to melt those edges, but not so hot that it burns through the thin root.
ISO 5817 limits for root imperfections, from the site table:
| No. | Imperfection | B — stringent | C — intermediate | D — moderate |
|---|---|---|---|---|
| 4021 | Incomplete penetration (lack of root penetration) | not permitted | not permitted | 0.2·t max 2 mm (short imperfections only) |
| 515 | Root concavity | 0.05·t max 0.5 mm | 0.1·t max 1 mm | 0.2·t max 2 mm |
| 504 | Excess penetration (b — root width) | 1 + 0.2·b max 3 mm | 1 + 0.6·b max 4 mm | 1 + 1·b max 5 mm |
For example, on 10 mm plate root concavity is limited to 0.5, 1 and 2 mm at B, C and D, and lack of root penetration is permitted only at D, as a short imperfection. Other thicknesses: ISO 5817 limits calculator.
Typical root defects and what to change
| Defect (ISO 6520-1) | Typical cause | What to change |
|---|---|---|
| Lack of penetration (402) | Gap closed by the tacks, root face too thick, electrode too large for the groove, travel too fast | Gap and root face to the table, re-measure after tacking, a smaller electrode, keep the keyhole open |
| Lack of fusion on one root face (4013) | Arc pointed at one side, misalignment, arc blow | Centre the arc on the gap, level the edges, see arc blow |
| Root concavity, suck-back (515) | Overhead section of a fixed pipe where the pool sags away; purge pressure too high; too much heat in the root | Shortest arc in the overhead part, lower purge pressure, less heat |
| Excess penetration (504) and burn-through (510) | Gap too wide, knife-edge root face, current too high, travel too slow | Root face 1–2 mm, gap inside the band, lower current or faster travel; a backing where the gap cannot be held |
| Oxidised, rough root on stainless | No purge or not enough purge | Back purge until the oxygen is low enough before striking, keep it on until the root has cooled |
| Slag at the root edges (301) | Root run not cleaned before the hot pass, humped root run | Grind the root run clean and flat before the hot pass |
Lack of penetration in detail, with nine causes: lack of penetration. Slag between the root and the hot pass: slag inclusions.
Standards and sources
This page adds no figures of its own. The numbers come from the tables of this site.
- ISO 9692-1, angle, gap and root face for the open root, as in the groove calculator and on joint preparation.
- ISO 5817, the limits for 4021, 515 and 504 from the site table on quality levels B, C, D.
- ISO 6520-1, imperfection numbers 402, 4013, 504, 510, 515 and 301, as in the ISO 6520-1 table.
- Current by electrode and position, the site’s current table with the position factors of the current calculator.
Frequently asked questions
What root gap and root face for a single-V butt weld?
Up to 12 mm: root face 1–2 mm, gap 2–4 mm for stick and TIG, 1–3 mm for MAG, with an included angle of 60° (stick), 50–60° (MAG) or 60–70° (TIG). Measure the gap after tacking.
What is the keyhole in root welding?
A small hole at the front of the pool where both root faces have melted through. It shows that the root is penetrating. Keep it the same size: if it closes there is no penetration, if it grows the root burns through.
What amperage for a 3.2 mm root?
The site table gives 90–140 A for 3.2 mm in the flat position, 75–120 A vertical up and 70–110 A overhead. Set it on a scrap piece with the same gap and root face; the root usually runs at the lower end.
Why is my root concave on the inside?
Typically in the overhead part of a fixed pipe, where the pool sags away from the root, or because the purge pressure pushes it up. Keep the arc shortest there, lower the purge pressure, and check against ISO 5817: on 10 mm, 0.5, 1 and 2 mm at B, C and D.
Do I need a backing bar for an open root?
Not if the gap and root face are right and you can hold the keyhole. A ceramic or copper backing helps where the gap varies, on long seams and with less experienced welders; permanent steel backing stays in the joint and the design has to allow for it.
How do I check the root from the inside of a pipe?
With a mirror at an open end or an endoscope through an opening, before the fill. Look for a continuous bead, both edges fused, no holes and no concavity.
Updated: